Prairie Stone International

Flexural Strength


Date3/20/2003 & 3/22/2003
Test MethodASDTM C99-87 (Reapproved 2000) Standard Test Method for Modulus of Rupture of Dimension Stone
Exposure CycleDryed at 60 +/-2 degrees C for 48 hours, then cooled to 23+/-2 degrees C in a desiccator
Support Span7 inches
Crosshead Speed0.02 inches/min (Dial @ 1.3)
Equipment Tinius Olsen, 10K pressure transducer ITS ID 9-0432
Mitutoyo Digital Calipers CD-18 SN 7003817
Mitutoyo Digital Calipers SN 98865 ITS ID 52639


Sample Length Width Thickness Max Load Modulus of Rupture
3/20/2003 (mm) (mm) (mm) (lbf) (MPa) (psi)
1202.0101.937.22762.33338
2201.0100.841.63882.65384
3201.7102.141.43092.10305
4201.3101.744.94962.88417
5202.6100.638.93863.02437
6201.4101.140.63222.30333
Mean Result2.54369
Coefficient of Variation14.2%14.2%


Sample Length Width Thickness Max Load Modulus of Rupture
3/22/2003 (mm) (mm) (mm) (lbf) (MPa) (psi)
1202.4102.239.64083.03439
2202.5101.842.43962.57373
3204.6101.842.12721.79260
4204.4101.343.83592.19318
5203.1102.342.74312.75399
6203.7101.838.71721.34195
Mean Result2.28331
Coefficient of Variation27.7%27.7%

PDF Format